Typical properties of unalloyed ductile cast iron
The table below shows the most important properties of ductile cast iron with spheroidal graphite.
| Grade designation | GGG 35.3 | GGG 40.3 | GGG 40 | GGG 50 | GGG 60 | GGG 70 | GGG 80 | GGG 90 |
| Matrix structure | ferritic | ferritic | predominantly ferritic | ferritic-pearlitic | predominantly pearlitic | pearlitic | pearlitic-sorbitic | |
| Tensile strength 1) (N/mm2) | 350 | 400 | 400 | 500 | 600 | 700 | 800 - 1000 | 900 - 1200 |
| Yield strength 2) 0.2 (N/mm2) | 220 | 250 | 280 | 350 | 420 | 500 | 570 - 700 | 650 - 800 |
| Elongation at break (%) | 22 | 18 | 15 | 7 | 2 | 2 | 7 | 4 |
| Brinell hardness HB 30 | 120 - 175 | 130 - 180 | 135 - 185 | 170 - 220 | 200 - 250 | 230 - 320 | 250 - 320 | 250 - 320 |
| Modulus of elasticity (N/mm2) | 165000 to 185000 | |||||||
| Compressive strength (N/mm2) | 650 - 500 | 700 - 900 | 800 - 1050 | 850 - 1100 | 1000 - 1200 | 1100 - 1300 | 1200 - 1400 | - |
| Flexural strength (N/mm2) | 700 - 850 | 750 - 900 | 800 - 900 | 850 - 1100 | 900 - 1200 | 1000 - 1300 | 1100 - 1400 | - |
| Compressive yield point (N/mm2) | approx. 1.2 times yield strength | |||||||
| Shear strength (N/mm2) | approx. 0.9 times tensile strength | |||||||
| Shear modulus (N/mm2) | 6500 to 6700 | |||||||
| Poisson's ratio | 0.28 to 0.29 | |||||||
| Rotating bending fatigue strength 2 (N/mm2) | 190 - 230 | 200 - 240 | 220 - 260 | 240 - 280 | 260 - 320 | 280 - 340 | 300 - 360 | 300 - 360 |
| Rotating bending fatigue strength 3) (N/mm2) | 120 - 160 | 120 - 160 | 120 - 160 | 140 - 180 | 160 - 200 | 160 - 200 | - | - |
| Impact bending strength 4) (RT) (N/cm2) | 100 - 180 | 100 - 180 | 80 - 160 | 60 - 120 | 40 - 80 | 20 - 60 | 20 - 40 | (20 - 40) |
| Notched impact strength 5) (RT) (N/cm2) | 14 | 14 | 10 | 3 | 0.8 | 0.7 | 0.6 | 0.5 |
2) ungekerbte Probe 3) gekerbte Probe, a=60°, Formzahl 3.1 4) ungekerbte DVM-Probe 5) DVM-Probe nach DIN 50112