Knowledge
Influence of alloying elements on cast iron
Typical properties of grey cast iron with lamellar graphite
| Alloying element | Rp | Rm | A | HB | increases/promotes | reduces/inhibits | Remark |
| Aluminium (Al) | - | - | promotes graphite degeneration (reduces tensile strength and yield strength, elongation) | inhibits surface formation of the spheroidal graphite | |||
| Lead (Pb) | - | - | promotes graphite degeneration (reduces tensile strength and yield strength, elongation) | inhibits surface formation of the spheroidal graphite | almost insoluble in iron; lead acts additively with bismuth in its disruptive effects | ||
| Chromium (Cr) | + | + | - | + | strongly carbide-forming (strong carbide former) | suppresses ferrite formation (even with slow cooling) | possible formation of insoluble carbide networks; to avoid carbide formation, the Cr content should be below 0.05% . Due to relatively high burn-off losses, add to the induction furnace relatively shortly before tapping. |
| increases the tendency to segregation | reduces the tendency of pearlite to decompose (during solidification and heat treatment) | ||||||
| promotes pearlite formation | |||||||
| Copper (Cu) | + | + | - | + | in the presence of Ti or Sn, even 1% Cu can result in graphite degeneration . | in the presence of disruptive elements, possibly graphite formation | Solubility is limited (approx. 4% in eutectic cast iron); with high Mg content, solubility only 1.5% (formation of Cu droplets); no risk of carbide formation; influence on the nodularisation of the graphite. Very low burn-off losses when alloying. |
| austenitisation (lowers the transformation temperature) | |||||||
| very strong pearlite-promoting effect | inhibits surface formation of the spheroidal graphite | ||||||
| Molybdenum (Mo) | + | + | - | weakly carbide-stabilising | narrows the austenite field | can have a ferritising effect at 0.1 to 0.3%; usually alloyed via ferromolybdenum, very low burn-off losses; yield is above 90%. | |
| promotes expansion of the ferrite halos | delays strongly the austenite transformation | ||||||
| at high Mo contents promotes the formation of bainite and martensite by suppressing pearlite formation | delays the pearlite transformation | ||||||
| extends the time window for martensite transformation (hardening) | lowers the Ms temperature | ||||||
| extends the time window for bainite transformation (hardening) | |||||||
| increases high-temperature strength | |||||||
| Nickel (Ni) | + | strong austenitisation (lowers the transformation temperature) | inhibits ferrite formation | 1% Ni lowers the austenitisation temperature by approx. 15 K; high Ni contents lead to bainite or martensite; no risk of carbide formation. High nickel contents can promote graphite degeneration. Alloyed using pellets; very low burn-off losses. | |||
| reduces the speed of the magnesium effect | |||||||
| increases the Cu solubility in ferrite | reduces the risk of embrittlement with high Cu additions | ||||||
| Titanium (Ti) | promotes graphite degeneration (reduces tensile strength and yield strength, elongation) | inhibits surface formation of the spheroidal graphite | |||||
| Tin (Sn) | - | + | strong pearlite former (approx. 13 times that of Cu) | used exclusively for pearlitic castings; add directly to the induction furnace shortly before tapping, as otherwise a temperature loss of approx. 20 K per 1% alloying element occurs. | |||
| promotes graphite degeneration (reduces tensile strength and yield strength, elongation) |